| Property | Unit | aPA | aPA 03 | 06 | MaPA | HaPA | Antistatic |
| Hardness (± 5°) | ShD | 82/76* | 78/72* | 76/71* | 76/71* | 82/76* | 82/76* |
| Min. tensile strength | N/mm | min. 45 | min. 40* | 35 | min. 35* | min. 45 | min. 45 |
| Min. ductility (± 10 %) | % | min. 40* | min. 40* | 50* | min. 50* | > 50 | > 20 |
| Charpy impact strength | kJ/m3 | 570 without breaking* | 470 without breaking* |
without breaking
without breaking*
|
570
without breaking*
|
570
without breaking*
|
| Notched impact strength | kJ/m3 | 3 10* | 4 10* | 38–12* | 38–12* | 25 | 4 |
| Density | g/cm3 | 1.15 | 1.15 | 1.14 | 1.14 | 1.14 | 1.16 |
| Friction coefficient *** | 0.30–0.35 | 0.25–0.30 | 0.22–0.27 | 0.30–0.35 | 0.30–0.35 | |
| Melting temperature | °C | 220 | 218 | 218 | 218 | 220 | 220 |
| Operating temperature | °C | -30 +80 | -30 +80 | -30 +80 | -30 +90 | -30 +90 |
| Longitudinal thermal expansion | °C | 8–10 . 10–5 | 9–11 . 10–5 | 9–11 . 10–5 | 8–10 . 10–5 | 8–10 . 10–5 | |
| Thermal conductivity | Wm-1K-1 | 0.30–0.35 | 0.28–0.35 | 0.28–0.35 | 0.30–0.35 | 0.30–0.35 | |
| Tensile e-modulus | MPa |
3200
1900*
|
3400–3700
2000–2500*
|
3600–3900
2100–2600*
|
3200
1900*
|
3200
1900*
|
| Equilibrium water content | % | 2.5* 7.2** | 2.5* 7.2** | 2.5* 7.2** | 2.5* 7.2** | 2.5* 7.2** |
| Relative change in linear dimensions | % | 0.85* 2.4** | 0.85* 2.4** | 0.85* 2.4** | 0.85* 2.4** | 0.85* 2.4** |

| Mechanical properties | ||
| Tensile strength at yield | ISO 527 | 80/50 MPa |
| Elongation | ISO 527 | 70/200 % |
| E-Modulus of tensile elasticity | ISO 527 | 3000/1500 MPa |
| Brinell Hardness | ISO 2039-1 | 150/70 MPa |
| Brinell Hardness Number | H358/30 | |
| Shore (A/D) or Rockwell (R/L/M) Hardness | ISO 868, ISO 2039-2 | D82/D68 |
| Izod notched impact strength at 23 °C | ISO 180/1A | 8.3/NB KJ/m2 |
| Charpy notched impact strength at 23 °C | ISO 179/1eA | 7/80 KJ/m2 |
| Electrical properties | ||
| Permittivity at 50 Hz | IEC 60250 | 4.0/12.0 |
| Permittivity at 1 MHz | IEC 60250 | 3.5/7.0 |
| Dielectric loss factor at 50 Hz | IEC 60250 | 100/3000 1E-4 |
| Dielectric loss factor at 1 MHz | IEC 60250 | 310/3000 1E-4 |
| Dielectric strength | IEC 60243-1 | 100/60 kV/mm |
| Thickness for dielectric strength | 0.6 mm | |
| Specific dielectric resistance | IEC 60093 | 1013/1010 Ωm |
| Surface resistance | IEC 60093 | 1013/1010 Ω |
| CTI Tracking resistance | IEC 60112 | 600 |
| Thermal properties | ||
| Thermal conductivity | DIN 52 612 | 0.23 W/K.m |
| Coefficient of transverse expansion, linear | ISO 11359 | 70|100 10-6/K |
| Melt or vitrification temperature | ISO 11357 | 220 °C |
| Heat distortion resistance A | ISO 75 HDT/A (1.8 MPa) | 65 °C |
| Heat distortion resistance B | ISO 75 HDT/B (0,45 MPa) | 160 °C |
| Max. short-term temperature | 180 °C | |
| Max. long-term temperature | 90 °C | |
| Min. operating temperature | -40 °C | |
| Other properties | ||
| Water absorption under regular conditions | ISO 62 | 3.0 % |
| Water absorption in humidity | ISO 62 | 9.5 % |
| Burning behaviour according to UL 94 | IEC 60695-11-10 HB | |
| UL 94 Thickness | 1.6 mm | |
| Special properties | ||
| Proportional elongation at yield | ISO 527 | 4/20 % |
| Tensile creep modulus (0.5% 1000 hrs) | ISO 899-1 | 2900/850 MPa |
| Flexural strength | ISO 178 | 125/60 MPa |
| Fatigue in flexure | ASTM D671 | 33 MPa |
| Izod impact strength at 23 °C | ISO 180/1C | NB/NB KJ/m2 |
| Izod impact strength at -30 °C | ISO 180/1C | NB/NB KJ/m2 |
| Charpy impact strength at 23 °C | ISO 179/1eU | NB/NB KJ/m2 |
| Charpy impact strength at -30 °C | ISO 179/1eU | NB/150 KJ/m2 |
| Coefficient of slip creep compared to steel | 0.38-0.45 | |
| Wear relative to the measured unit | 9.5 (µ m/km)/MPa | |
| CTI M Tracking resistance | IEC 60112 | 600M |
| Specific heat capacity | IEC 1006 | 1.70 J/g K |
| Vicat softening point B | ISO 306 VST/B/50 (50 N) | 204 °C |
| LOI Acid index | ISO 4589 | 25 % |

| Mechanical properties | ||
| Tensile strength at yield | ISO 527 | 90/60 MPa |
| Elongation | ISO 527 | 20/60 % |
| E-Modulus of tensile elasticity | ISO 527 | 3600/2100 MPa |
| Brinell Hardness | ISO 2039-1 | 160/90 MPa |
| Brinell Hardness Number | H358/30 | |
| Shore (A/D) or Rockwell (R/L/M) Hardness | ISO 868, ISO 2039-2 D83/D71 | |
| Izod notched impact strength at 23 °C | ISO 180/1A | 7.0/NB KJ/m2 |
| Electrical properties | ||
| Permittivity at 1 MHz | IEC 60250 | 3.7 |
| Dielectric loss factor at 1 MHz | IEC 60250 | 300/- 1E-4 |
| Dielectric strength | IEC 60243-1 | 100/50 kV/mm |
| Thickness for dielectric strength | 0.6 mm | |
| Specific dielectric resistance | IEC 60093 | 1013/1010 Ωm |
| Surface resistance | IEC 60093 | 1012/1010 Ω |
| CTI Tracking resistance | IEC 60112 | 600 |
| Thermal properties | ||
| Thermal conductivity | DIN 52 612 | 0.29 W/K m |
| Coefficient of transverse expansion, linear | ISO 11359 | 80 10-6/K |
| Melt or vitrification temperature | ISO 11357 | 220 °C |
| Heat distortion resistance A | ISO 75 HDT/A (1.8 MPa) | 120 °C |
| Heat distortion resistance B | ISO 75 HDT/B (0,45 MPa) | 185 °C |
| Max. short-term temperature | 150 °C | |
| Max. long-term temperature | 80 4) °C | |
| Min. operating temperature | -40 °C | |
| Other properties | ||
| Water absorption under regular conditions | ISO 62 | 2.8 % |
| Water absorption in humidity | ISO 62 | 8.0 % |
| Burning behaviour according to UL 94 | IEC 60695-11-10 | V-2 |
| UL 94 Thickness | 3.2 mm | |
| Special properties | ||
| Tensile creep modulus (0.5% 1000 hrs) | ISO 899-1 | 2300/1000 MPa |
| Flexural strength | ISO 178 | 140/70 MPa |
| Izod impact strength at 23 °C | ISO 180/1C | NB/NB KJ/m2 |
| Izod impact strength at -30 °C | ISO 180/1C | NB/NB KJ/m2 |
| Coefficient of slip creep compared to steel 0.36 to 0.43 | ||
| Wear relative to the measured unit | 6.3 (µm/km)/MPa | |
| CTI M Tracking resistance | IEC 60112 | 600M |
| Specific heat capacity | IEC 1006 | 1.68 J/g K |
| Vicat softening point B | ISO 306 VST/B/50 (50 N) | 215 °C |
| LOI Acid index | ISO 4589 | 25 % |